来源:http://www.jnghbxg.com 日期:2026-11-16 发布人: 浏览次数:1次

济南做轻型钢结构,最容易翻车的地方不是屋顶漏雨、不是墙面不平,是柱脚。混凝土基础浇完、钢柱立上去、外包板一封,里面锈成什么样谁也不知道。等三年后整排柱子往一边歪,拆开一看柱脚截面啃掉三分之一。

The most prone area for a light steel structure to overturn in Jinan is not roof leaks or uneven walls, but column bases. After the concrete foundation is poured, the steel columns are erected, and the outer cladding is sealed, no one knows what kind of rust has formed inside. After three years, the entire row of columns will tilt to one side, and upon opening, one-third of the column base section will be gnawed off.

柱脚防腐是隐蔽工程里的隐蔽工程

Column base anti-corrosion is a concealed project in concealed engineering

锚栓预埋时,螺纹段要缠胶带保护不被混凝土糊死,但杆身和底板接触面必须做防腐处理——环氧富锌底漆+厚浆型面漆,干膜总厚≥200μm。很多施工队只刷一遍灰漆甚至不刷,理由是"埋在混凝土里又淋不到雨"。错。混凝土毛细吸水,济南地下水位浅、融雪剂渗透,柱脚底部是电化学腐蚀最活跃的区域。

When embedding anchor bolts, the threaded section should be wrapped with tape to protect it from being stuck by concrete, but the contact surface between the rod body and the bottom plate must be treated with anti-corrosion treatment - epoxy zinc rich primer+thick paste topcoat, with a total dry film thickness of ≥ 200 μ m. Many construction teams only brush gray paint once or even do not brush it, citing the reason that it is "buried in concrete and cannot be exposed to rain". wrong. Concrete capillary water absorption, shallow groundwater level in Jinan, infiltration of snow melting agents, and the bottom of the column base are the most active areas for electrochemical corrosion.

1

锚栓选型和预埋精度

Anchor bolt selection and pre embedding accuracy

M24以上优先用双螺母+垫圈,外露螺纹留2–3扣,不缩进去也不冒太长;

Priority should be given to using double nuts and washers for M24 and above, leaving 2-3 threads exposed without shrinking or extending too much;

预埋定位偏差≤5mm,超了钢柱底板孔对不上,现场气割扩孔直接废掉节点强度;

The pre embedded positioning deviation is ≤ 5mm, which exceeds the steel column bottom plate hole and cannot be aligned. On site gas cutting and hole expansion directly invalidate the node strength;

柱脚底板与基础顶面留50–80mm二次灌浆层,用无收缩灌浆料填实,不塞砂浆;

Leave a 50-80mm secondary grouting layer on the bottom plate of the column base and the top surface of the foundation, and fill it with non shrink grout without adding mortar;

抗剪键(抗剪槽)必须做,纯靠锚栓抗剪会剪断螺纹。

Anti shear keys (anti shear grooves) must be made, relying solely on anchor bolts to resist shear will cut the threads.

二次灌浆是命门

Secondary grouting is the gateway to life

灌浆料选CGM类无收缩型,流动度≥300mm,24小时强度≥30MPa。灌浆前基础面凿毛、清水润湿无明水,从一侧灌入排气,不分段塞。灌完养护7天再紧螺母。偷懒用普通水泥砂浆,收缩开裂进水,柱脚直接泡在泥浆里生锈。

The grouting material should be CGM non shrink type, with a flowability of ≥ 300mm and a 24-hour strength of ≥ 30MPa. Before grouting, the foundation surface should be chiseled and moistened with clean water without visible water. Exhaust should be injected from one side without segmented plugging. After filling and curing for 7 days, tighten the nut. Lazy use of ordinary cement mortar leads to shrinkage, cracking, and water ingress, causing the column base to rust directly in the mud.

济南本地特别注意

Jinan local special attention

回填土区域基础必须做独立承台+拉梁,不靠地面硬化层传力;

The foundation of the backfill soil area must be built with independent bearing platforms and tension beams, without relying on the ground hardening layer for force transmission;

冻土层1.2–1.5米,基础埋深必须过冻土线,不然春天一化一冻柱子往上拱;

The frozen soil layer is 1.2-1.5 meters deep, and the foundation burial depth must pass through the frozen soil line, otherwise in spring, the frozen column will arch upwards;

天沟落水管别正对柱脚排,雨水顺着柱子流到基础根部,不锈钢天沟也要接雨水管引走。

The downspout of the gutter should not be directly facing the column base, and rainwater should flow along the column to the base of the foundation. The stainless steel gutter should also be connected to the rainwater pipe for drainage.

验收时柱脚区域要拍照片留存:防腐涂层厚度、灌浆密实度、螺母紧固扭矩、抗剪键位置。这些以后埋进地面就看不到了,出问题没有追溯依据。

During acceptance, photos should be taken of the column base area for retention: thickness of anti-corrosion coating, grouting density, tightening torque of nuts, and position of shear keys. These will no longer be visible when buried on the ground, and there will be no trace basis for any problems.

轻钢厂房的寿命,屋顶撑15年,柱脚决定能不能撑30年。基础以上做得再漂亮,柱脚烂了整栋推倒重来。

The lifespan of a light steel factory building is determined by whether the roof can support for 15 years and the column base can support for 30 years. No matter how beautiful the foundation is, if the column base is broken, the whole building will be demolished and rebuilt.